Aug 16, 2022 Leave a message

Process Control Of Double Wave Soldering Machine

1. Flux spraying

Paste a piece of white paper on the PCB with double-sided tape, and apply the flux to check whether the flux is sprayed evenly, whether it is leaking, and whether the flux enters the hole, especially the OSP hole. Missing spray is often a common cause of bridging and sharpening.

2. Preheating

Preheating serves the following purposes:

(1) Volatilize most of the flux to avoid splashing during soldering and cause the temperature of the tin wave to drop (because the volatilization of the flux requires heat absorption).

(2) Obtain proper viscosity. If the viscosity is too low, the flux is easily taken away by the tin wave prematurely, which will make the wetting worse;

(3) Obtain the proper temperature. Reduce thermal shock and board deformation when PCBA enters solder wave;

(4) Promote flux activation.

3. Judgment of suitable preheating results

(1) For leaded soldering, the soldering surface is about 110°C. For a given PCBA, it can be judged by measuring the temperature of the component surface; it can also be touched by hand, and it can be sticky. Too dry it will easily cause soldering problems.

(2) For the OSP board, the preheating temperature needs to be appropriately increased, such as 130°C.

(3) ENIG board, depending on whether single wave or double wave is used. Dual waves require higher preheat temperatures, while single waves require lower preheat temperatures to avoid pad edge dewetting.

4. Wave soldering

(1) The upward turbulent wave should have a certain impact force, forming irregular valleys and peaks;

(2) The smooth wave tin wave surface must be flat, and the wave height is adjusted to achieve defect-free welding.

Different waveforms have different requirements. For example, a certain brand of wave soldering machine, when the wave ratio is low, there are more bridges and tips (insufficient heating); when the wave ratio is high, the fullness of the solder joints will become worse (rapid pull-down). These are based on its narrow arc-shaped wave characteristics. Pulling the tip, usually because the solder has not been pulled down and the upper part has solidified. The reason for solidification is that the lead heat dissipation is faster or the lead wire is relatively long. In order to avoid sharpening, it is sometimes necessary to smooth the wave pressure deeper to increase the heat capacity of the lead wire. It can also be achieved by reducing the transmission speed (under the premise of high-speed transmission).

The adjustment of the wave height must be adjusted according to the transmission speed, and it is often difficult to achieve the goal by simply adjusting the wave height. Conveying speed: affects the heating and separation speed of the solder joints. Generally, it cannot be adjusted separately, and needs to be adjusted according to the waveform and the PCBA being welded.